An AGV showing 35% battery still stalls on a ramp because pack resistance grew from 28 to 65 milliohms
A 48 V, 100 Ah lithium-iron-phosphate pack on an underride AGV ran for 14 months on a fixed loop, eleven hours a day. Then it began stopping at the bottom of a 3-degree ramp with the dashboard still reading 35 percent. The vehicle was not broken in any obvious way: lidar navigation, servo control and PLC diagnostics all reported healthy, and positioning stayed within plus or minus 8 millimetres. It simply could not climb.
The first response on site was to swap the battery management system twice, reflash firmware three times, and relax the undervoltage cutoff from 2.80 V to 2.60 V per cell. Those moves only moved the failure point from 35 percent to 28 percent. The pack was not low on charge. Its internal resistance had climbed from 28 milliohms when new to 65 milliohms, and at 150 A of climb current that resistance dropped the terminal voltage by 9.75 V, pulling a cell below the 2.80 V protection line.
Three clues that point at the same thing
The stop happened three times a day, always at the same ramp, always with the dashboard near 35 percent. On flat ground it ran all day without a single event. Three observations narrow the cause quickly.
First, the stop occurs only during the three seconds of peak current. The 3-degree ramp with an 800 kg load draws 150 A; flat cruising draws 60 A.
Second, the terminal voltage at the moment of the stop was recorded: 39.5 V, while the dashboard reported 35 percent and 49.2 V.
Third, after the vehicle sat for 30 minutes with no load, the dashboard still read 35 percent and the terminal voltage returned to 49.2 V, identical to before.
A loaded reading of 39.5 V and an unloaded reading of 49.2 V differ by 9.7 V that is not stored anywhere in the battery. It is consumed on the spot by current flowing through resistance.
The meter is not wrong, it is reading the wrong place
The dashboard estimates state of charge from open-circuit voltage measured after a rest, a method called OCV lookup. That estimate is correct: after 30 minutes of rest the pack genuinely sits at 35 percent, 49.2 V across 15 cells or 3.28 V each. The problem is that the vehicle never stops to let the meter look up the table. The instant it is under load, terminal voltage is no longer open-circuit voltage.
Step one: rest thirty minutes and compare two numbers
Park the vehicle, remove all load, wait 30 minutes, then read the dashboard state of charge and measure the real terminal voltage with a multimeter.
If the dashboard says 35 percent and the meter reads 49.2 V, the meter is right and the fault is downstream in the power path. If the dashboard says 35 percent but the meter reads only about 45 V, a few cells have fallen behind and the issue is pack consistency, not resistance.
This step takes one multimeter and five minutes and tells you which direction to look.
Step two: watch the terminal voltage under load
Clip the multimeter across the pack output, not the distribution-box entry, then make the vehicle climb the ramp or start against a heavy load and watch the lowest reading.
A drop under 4 V means resistance is normal and the cause is elsewhere. A drop over 8 V means resistance has already grown large, and that is the case this article describes.
Probe placement matters. Measuring at the distribution-box entry captures battery drop plus harness drop; measuring at the pack terminals captures only the battery. If the two readings differ by more than 1 V, the cabling is also stealing voltage.
Step three: compute one resistance
Resistance is the open-circuit voltage minus the loaded voltage, divided by the current at that moment. In the 39.5 V event:
R = (49.2 - 39.5) / 150 = 64.7 milliohms
The factory value was 28 milliohms. The same pack had grown 2.3 times. No teardown, no host-computer session, the fault is characterised.
The mechanism: Ohm's drop U equals OCV minus I times R
One equation, three variables. Open-circuit voltage is set by state of charge, resistance by battery age and temperature, and current by the duty cycle. Of the three, only open-circuit voltage is visible on the dashboard. The cutoff is simple: when any cell drops below 2.80 V, the BMS disconnects. Across 15 cells that is a pack voltage of 42.0 V.
A new pack at 28 milliohms survives all three duty points at 35 percent state of charge, where open-circuit voltage is 49.2 V:
| Duty | Current | Terminal | Per cell |
|---|---|---|---|
| Flat cruise | 60 A | 49.2 - 1.68 = 47.5 V | 3.17 V |
| Ramp climb | 150 A | 49.2 - 4.20 = 45.0 V | 3.00 V |
| Startup surge | 200 A | 49.2 - 5.60 = 43.6 V | 2.91 V |
The lowest cell is 2.91 V, 0.11 V above the 2.80 V line. A new pack will not trip at this charge level no matter what it does.
The aged pack at 65 milliohms trips on two of the three:
| Duty | Current | Terminal | Per cell |
|---|---|---|---|
| Flat cruise | 60 A | 49.2 - 3.90 = 45.3 V | 3.02 V (pass) |
| Ramp climb | 150 A | 49.2 - 9.75 = 39.5 V | 2.63 V (trip) |
| Startup surge | 200 A | 49.2 - 13.0 = 36.2 V | 2.41 V (trip) |
Only 37 milliohms separate the two packs, yet the old one runs fine on the flat and stalls on the ramp. That is exactly why this fault is mistaken for an occasional glitch.
Why a two-volt difference looks like twenty percent of charge
Lithium iron phosphate is famously flat. Between 20 and 80 percent state of charge a single cell moves from 3.26 V to 3.33 V. Sixty percentage points span only 70 millivolts. Across the 15-cell pack the entire plateau is just 1.05 V.
The aged pack's 3.90 V flat-load drop is 3.7 times wider than the whole plateau. The practical consequence is that under load the terminal voltage carries almost no information about remaining charge. You cannot work backward from 39.5 V to a state of charge; it might correspond to 5 percent or to 50 percent.
The dashboard still dares to show 35 percent because the BMS does not look up charge directly from terminal voltage. It seeds the value from open-circuit voltage at rest, then counts ampere-hours down during load, and the two correct each other. That algorithm is stable, so the 35 percent is probably real. It is not wrong. It simply does not know its own resistance has grown.
Where the 65 milliohms comes from
Measured per source on the same pack:
| Source | New | After 14 months | Change |
|---|---|---|---|
| 15 cells | 18.0 mΩ | 48.0 mΩ | +30.0 |
| Copper busbars and posts | 5.0 mΩ | 8.0 mΩ | +3.0 |
| Harness and terminals | 3.0 mΩ | 3.0 mΩ | 0 |
| Contactor contacts | 2.0 mΩ | 6.0 mΩ | +4.0 |
Of the added 37 milliohms, the cells contribute 30, or 81 percent. Contactor erosion adds 4, busbar oxidation adds 3.
The most common field reaction is to replace the contactor, thicken the harness and polish the posts. Those three together recover at most 7 milliohms, taking the pack from 65 to 58 milliohms. The drop then falls from 9.75 V to 8.7 V, the per-cell voltage to 2.70 V, and it still trips.
Cell resistance grows 2.7 times for three overlapping reasons: the solid-electrolyte-interphase film thickens as part of normal aging, long storage at high state of charge accelerates calendar aging, and a summer workshop at 38 degrees Celsius with the pack fully charged at rest roughly doubles the aging rate for every 10 degrees. A 100 Ah pack after 14 months and about 700 cycles reaching 48 milliohms in the cells is not abnormal. It is not broken. It is simply old.
Three duties, two packs, who trips
| Duty | Current | New 28 mΩ | Aged 65 mΩ |
|---|---|---|---|
| Flat cruise | 60 A | 47.5 V / 3.17 V | 45.3 V / 3.02 V (pass) |
| Ramp 3 deg | 150 A | 45.0 V / 3.00 V | trips |
| Startup surge | 200 A | 43.6 V / 2.91 V | trips |
The ramp is the failure because it is the only duty that combines the largest current with a duration longer than three seconds. The startup surge is larger but lasts only 0.4 seconds; the BMS undervoltage delay of one second never elapses, so the pack recovers. The ramp lasts more than ten seconds, the delay expires, and the contactor opens.
Usable capacity at 90 Ah (the 100 Ah pack derated 10 percent) means the aged pack is cut off at 35 percent and actually delivers only 58.5 Ah. Range falls from 3.6 hours to 2.3 hours, a 35 percent loss. The operator feels a vehicle that runs out sooner; the report shows rising charge frequency. Both symptoms share one root.
Five mistakes, in the order teams make them
Mistake one is replacing the BMS without measuring resistance. The BMS is a passive protector; its undervoltage report is true. Swapping the board is disconnecting the alarm while the vehicle still stalls.
Mistake two is lowering the undervoltage threshold. Moving it from 2.80 V to 2.60 V shifts the stop from 35 percent to 28 percent and looks fixed. The cost is cells repeatedly discharged to 2.6 V, where lithium plating risk climbs and the next 14 months shorten. This trades life for time.
Mistake three is thickening the harness to cut the drop. The harness is only 3 milliohms; doubling it saves at most 1.5 milliohms and 0.2 V, while the 30 milliohms in the cells is untouched. The only effective lever is peak current, covered next.
Mistake four is ignoring temperature. At minus 10 degrees Celsius resistance scales by 2.2, taking the aged pack from 65 to 143 milliohms. At the same 150 A the drop becomes 21.5 V, the terminal 27.7 V and the per-cell voltage 1.85 V; the vehicle stalls before it can even alarm. Northern sites must re-measure resistance before winter rather than carry summer numbers year-round.
Mistake five is watching state of charge but never state of health. The dashboard shows capacity and nothing about health. The fleet backend should chart resistance or state of health weekly. Resistance rising from 28 to 40 milliohms is the moment to warn, while replacement can still be scheduled. At 65 milliohms the cost is a line stoppage.
Working with the navigation layer: report charge early, do not stall in the aisle
Current limiting beats speed limiting. The aged pack fears the few seconds above 150 A. Two limits tell the story:
Limiting to 120 A gives a 7.8 V drop, a 41.4 V terminal and 2.76 V per cell, still below 2.80 V, still tripping. Limiting to 100 A gives a 6.5 V drop, a 42.7 V terminal and 2.85 V per cell, safe. The boundary is not "limit a little"; it sits on the 42.0 V line. Current must fall below 100 A to keep 0.7 V of margin.
The price is climb speed dropping from 0.6 to 0.4 metres per second, adding about five seconds to that ramp. Five seconds to avoid a stall is worth it.
The recharge threshold should track resistance. The default 20 percent recharge is too low for the aged pack, which cannot deliver peak current even at 35 percent. Working backward, safely passing 150 A needs open-circuit voltage above 42.0 + 150 times 0.065 = 51.75 V, or 3.45 V per cell. Full charge only reaches 3.40 V, so the aged pack has no safe state-of-charge window at 150 A at all; raising the threshold cannot rescue it. A resistance-based recharge threshold reduces low-state-of-charge climbs but does not replace current limiting.
Do not let positioning take the blame. The most common misdiagnosis is "positioning drifted, navigation is unstable." Positioning precision never changed; the vehicle simply stopped before reaching the point. The distinction is trivial: read the fault code at the stop. Undervoltage protection leaves a record; a positioning loss does not.
Three steps to tell meter wrong from pack old
First, rest 30 minutes and compare: if the dashboard state of charge and the measured voltage agree, the meter is correct. Second, watch the loaded voltage drop: a fall over 8 V while climbing means resistance is large. Third, compute R = (OCV - U) / I and if it exceeds 1.5 times the factory value, replace the pack. Do not change the BMS, do not adjust the threshold, do not thicken the harness.
Whether an AGV battery should be replaced should be decided by its resistance curve, not by how far it runs before stalling. Record resistance in the maintenance ledger and this class of stoppage stops being treated as an occasional fault.
Source: RANKING IOT (Suzhou Yunqi Intelligent Technology), WeChat, 4 November 2026.